Salt cementation reaction


It´s a classic reaction, invented by Lydians in ancient times of 7th...6th century BC, and the source of money of the world.

What happens?

The basic reaction is

Ag + NaCl + ??? -> AgCl + ???

How can the reaction ever go ahead?
I don´t expect Ag, let alone a small impurity of Ag in Au, to displace metal Na.
So you need oxidant. What is it?
Where does Na go?
Important basis for it is differential reactivity of Au and Ag. Au does form chlorides at low temperature under influence of aqua regia or chlorine, but those decompose to metal on heating to about 300 Celsius. AgCl melts at 450 and endures over 1000 Celsius without melting.
So what are the ??? reagents and products above? What is the temperature range?
Pt forms PtCl2 that melts at 581 Celsius. When gold contains appreciable amounts of Pt alongside Ag, does Pt partition into the chloride phase or remain in metal?
View user's profile View All Posts By User
Texium
Administrator
********




Posts: 4546
Registered: 11-1-2014
Location: Salt Lake City
Member Is Offline

Mood: PhD candidate!

[*] posted on 16-5-2020 at 08:13


From a quick google of the subject, it appears that this process was not typically carried out using only salt. As with nearly all ancient chemistry from before there was a good understanding of elements and compounds, there are many variations, and most of them involve very complex mixtures. Typically these gold parting mixtures included salt alongside urine or a soil especially rich in nitrates and/or ammonium salts. This of course would lead to a cyclic process of the silver being leached out of the mixture by formation of silver nitrate or a silver ammine complex, and the solubilized silver being precipitated as AgCl. Then it's roasted at high temperatures to recover (substantially more) pure molten gold and vapors of AgCl which are deposited and further refined to pure silver metal.



Come check out the Official Sciencemadness Wiki
They're not really active right now, but here's my YouTube channel and my blog.
View user's profile Visit user's homepage View All Posts By User
chornedsnorkack
National Hazard
****




Posts: 552
Registered: 16-2-2012
Member Is Offline

Mood: No Mood

[*] posted on 16-5-2020 at 08:54


In this
https://chemistry.stackexchange.com/questions/55734/how-were...

Berthelot is quoted as referring to "calcined red vitriol" as an ingredient.
Is it Fe2O3? Or Fe2(SO4)3?
View user's profile View All Posts By User
Fulmen
International Hazard
*****




Posts: 1701
Registered: 24-9-2005
Member Is Offline

Mood: Bored

[*] posted on 17-5-2020 at 00:32


Did you even try to research this? from Wikipedia:

Hoover and Hoover[16] explains the process thus: under heating salt (sodium chloride, NaCl) decomposes in the presence of silica and alumina (from the brick dust or clay) to produce hydrochloric acid and also some chlorine. This reacts with the silver to produce silver chloride (AgCl).




We're not banging rocks together here. We know how to put a man back together.
View user's profile View All Posts By User
chornedsnorkack
National Hazard
****




Posts: 552
Registered: 16-2-2012
Member Is Offline

Mood: No Mood

[*] posted on 17-5-2020 at 02:50


Quote: Originally posted by Fulmen  
Did you even try to research this? from Wikipedia:

Hoover and Hoover[16] explains the process thus: under heating salt (sodium chloride, NaCl) decomposes in the presence of silica and alumina (from the brick dust or clay) to produce hydrochloric acid and also some chlorine. This reacts with the silver to produce silver chloride (AgCl).


Yes, I tried just that! And the Wikipedia made absolutely no sense. Because silica and alumina are not oxidants and do not contain hydrogen. The reaction
4NaCl+SiO2->4HCl+???
is flagrantly impossible because no H atoms on the left side.
Reaction
4 NaCl+SiO2-> 2Cl2+???
also absurd. No oxidant on the left strong enough to produce an oxidant as strong as elementary chlorine.
View user's profile View All Posts By User
Boffis
International Hazard
*****




Posts: 1848
Registered: 1-5-2011
Member Is Offline

Mood: No Mood

[*] posted on 17-5-2020 at 04:16


It is a curious and well known phenomina that salt attacks silver, that's why silver dining services used to have a glass liner inside the salt cellars. I have often wonder about how this reaction occurs and its precise chemistry. It is worth noting that AgCl is not decomposed by aqueous alkalis and therefore I suspect that the atmospheric oxygen and water are important reactant and the reaction occurs alone the lines of:

2Ag + 2NaCl + H2O + O -> 2NaOH + 2AgCl

The highly insoluble nature of the silver chloride driving the reaction by removing the silver ions. The NaOH then absorbs CO2 or some other acid moiety preventing the reversal of the reaction. This reaction occurs spontaneously at room temperature probably using water gathered from the air by the hydroscopic salt meaning that the salt grains become covered with a layer of saturated salt solution.

I don't know if this reaction works at high temperatures but I suspect that something similar will. Given that in ancient times most ores mined were from the oxide zone and rich in Fe3+ and Mn4+ as well as silica I can imagine that a reaction such as:

2Ag + 2NaCl + Fe2O3 + 2SiO2 -> Na2SiO3 + 2AgCl + Fe2SiO4

would occur. The iron silicate is called fayalite and, from personal experience, is a very common component of ancient slags. I once worked on a project to recovery copper and precious metal from ancient slags in Turkey that were more than 3500yrs old and consisted mainly of fayalite and glass in which occurred tiny prills of copper alloy.

I am not sure how this would help the ancient but maybe they could leach the AgCl out of the matt with lime and urine (ammonia) and then cement the silver onto copper. Or perhaps molten silver chloride is simply immiscible with the silicate melt and separates out.
View user's profile View All Posts By User
chornedsnorkack
National Hazard
****




Posts: 552
Registered: 16-2-2012
Member Is Offline

Mood: No Mood

[*] posted on 17-5-2020 at 06:04


Yes. If "calcined red vitriol" were Fe2(SO4)3 then the reactions could go:
Fe2(SO4)3+6NaCl->3Na2SO4+2FeCl3
FeCl3 melts and then boils slightly over 300 Celsius
And is reasonably strong oxidant to attack Ag:
FeCl3+Ag->FeCl2+AgCl
View user's profile View All Posts By User