Sciencemadness Discussion Board

Decent cell build....

markx - 15-2-2019 at 08:14

I finally got fed up with the halfbaked solutions and contraptions that I've been using as an excuse for a cell regarding electrosynthesis of chlorate and perchlorate.
It is time to create a worthy vessel to contain the process better and not stink up the room or cover it in salt residue. Not to mention the zombie outbreak of corrosion that follows...

So.....a "huge" beaker shaped glass vase is chosen as the main vessel for the electrolyte. It is cheap, functional and replaceable.
Now we begin to machine the flanges that shall encase the vase from bottom and top, containing all the goodies inside.
Titanium rod is machined to make the electrode stems....drilled...tapped. Oh it is fun to tap a blind hole in Ti :D !

IMG_3173.JPG - 819kB IMG_3176.JPG - 680kB IMG_3181.JPG - 817kB IMG_3184.JPG - 637kB IMG_3186.JPG - 611kB IMG_3187.JPG - 694kB


It is taking shape. The flanges are made from PP plastic and grooved to fit the lip of the vase against a gasket and also the bottom is sitting in recess for correct centering and stability:

IMG_3189.JPG - 655kB IMG_3190.JPG - 681kB



Into the top flange three ports are installed as threaded inserts. For leading away the formed gases....for sampling of electrolyte.....and for holding a glass thermometer in place. The thermometer port has an adjustable ptfe gasket that gently grabs and seals the outer perimeter of the glass tube.
Also proper fasteners are machined and oxide coated to tighten the flanges on the treaded rods:

IMG_3199.JPG - 534kB IMG_3201.JPG - 625kB IMG_3201.JPG - 625kB



Almost operational:

IMG_3202.JPG - 573kB IMG_3204.JPG - 564kB IMG_3205.JPG - 600kB

The cell was fitted with a slightly but passionately used set of electrodes (MMO/ Ti) for chlorate synthesis. Just some details to take care of before we can fill it up and turn the current on.
Gotta direct the gas flow to outside and find/make a gasket to seal the upper flange against the lip of the vase reliably.
That should prevent the gasses and salt spray from exiting anywhere but through the off gas port and make the process much more pleasant for the surroundings.

DavidJR - 15-2-2019 at 09:23

Nice work!

Ubya - 15-2-2019 at 09:39

Well done.
how many things i could make if i had the space and money (but mostly the space) to have a lathe, a drill press and a few other things.

ps the vase could be wrapped with a heating cord to make a heated cell (for chlorate production)

markx - 17-2-2019 at 14:05

We are in business....and the air is clean :)

IMG_3211.JPG - 566kB IMG_3212.JPG - 439kB IMG_3213.JPG - 616kB

I must fit a plastic vessel under the cell to contain the fluid if the vase should break. I can already see it happening....





markx - 19-2-2019 at 13:21

The contraption has been operating with NaCl solution (1kg charge in the vessel) for about 48 hours now....seems to work quite stable, clean and smooth:


IMG_3220.JPG - 471kB



IMG_3218.JPG - 904kB

The temperature hovers around 70-75C with no extra cooling or heating and the current is at about 27-30A with 4V applied across the electrodes. Considerable amount of ClO3- has been generated, assessed by the amount of crystals forming when a liquor sample is mixed with KCl solution. There is minimal salt creep from the connections...I trust there would be virtually none if the gas exhaust would not have become blocked during the first 12h of operation. That generated pressure in the cell and forced the liquid through the fittings. I used a too small exhaust tube and tried to lead it straight out into the cold winter weather.....of course the salt spray and water vapour collected into the tube, were forced out to the cold and there they assumed it would be a good idea to block the tube and move no further. I kind of thought that would happen, now it's has been proven. So I just chucked the tube into a bottle of water beside the reactor and called it good. There is virtually no smell at all...just a steady stream of H2 bubbles coming out of the exhaust tube. That can of course be changed into a radical chlorine stench if I should decide to mess with pH control :D
But naaah....too much hassle, I just let it run it's course and do nothing of the sort.

markx - 23-2-2019 at 04:54

Finished the first stage of the conversion from Cl- to ClO3- in five days. I suspect it was pretty much done on the fourth day already. Current started dropping off slightly and temps went up to almost 80C.

Cell was dismantled cleaned from salt creep and fitted with a homemade Pt coated Ti anode for the next step of conversion from ClO3- to ClO4-

The anode was made by coating a previously sanded and cleaned Ti sheet with a thin layer of hexachloroplatinic acid solution which was thermally decomposed in a kiln at 350C to yield a coating of metallic Pt. I suspect the decomposition temperature was a bit on the high side, but it worked nicely.

IMG_3223.JPG - 484kB IMG_3222.JPG - 499kB IMG_3227.JPG - 827kB IMG_3229.JPG - 772kB IMG_3224.JPG - 731kB IMG_3221.JPG - 546kB

It's ticking along with a quiet fizzing and the temp holds stable at 50C.




IMG_3226.JPG - 433kB

Sulaiman - 24-2-2019 at 01:44

Nice work

I do not like the hazard of many amps-worth of hydrogen gas being continuously discharged,
but I do not have a simple solution to offer.

Generally, electrolysis tends to produce various valuable waste gasses,
(hydrogen, oxygen, chlorine ..)
my puny electrolysis experiments are more for learning than producing,
but you may find a good use for by-products ?
(hydrogenate, oxidise, chlorinate .. something, hydrogen balloon ?)
just a thought.

P.S. Keep a look out for a spare/replacement glass vessel :P

[Edited on 24-2-2019 by Sulaiman]

markx - 24-2-2019 at 12:45

Quote: Originally posted by Sulaiman  
Nice work

I do not like the hazard of many amps-worth of hydrogen gas being continuously discharged,
but I do not have a simple solution to offer.

Generally, electrolysis tends to produce various valuable waste gasses,
(hydrogen, oxygen, chlorine ..)
my puny electrolysis experiments are more for learning than producing,
but you may find a good use for by-products ?
(hydrogenate, oxidise, chlorinate .. something, hydrogen balloon ?)
just a thought.

P.S. Keep a look out for a spare/replacement glass vessel :P

[Edited on 24-2-2019 by Sulaiman]


30A worth of hydrogen shall hardly contribute to a rise in hazard level. Besides I do lead it outside....or at least that was the original intention. But winter conditions got in the way and since it is more of a trickle than an outpour, I just let it rise to the ceiling and out the cracks.

Gathering and storing it is not a viable practice.....there is not so much, it is contaminated by chlorine, oxygen and probably several more things. So of little worth in most instances. And it likes to creep out of containment anyways.

According to my practice the glass vessels last a very long time.....that is if one does not break them :D
But even in that case they are like 3$ a pop in local "walmart" so not to worry. And there are even specimens about three times the volume of this one available for asocial prices too.

Sulaiman - 24-2-2019 at 13:59

excellent - all covered.

I'm still only at the dreaming stage re. making suitable anodes :(

markx - 2-3-2019 at 02:22

Aaaargh.....jesus, what a cluster***k!



DSCF1922.JPG - 1.1MB

The whole thing went to hell on a greased rail. From the beginning of the perchlorate stage I felt that the cell was not acting quite the way it should have. Anode was just holding up too good and I saw no signs of passivation or current dropping within the first five days. Which in all honesty is not a bad thing, had it not been accompanied by absolutely zero ClO4- forming. So I started to ramp up the voltage to about 5V and all that happened was a quickly passivating anode which caused a massive polarisation that was high enough to start corroding the anode current collector. Seems it was composed of a Ti alloy that does not hold up to high anodic potential. The mess of white percipitate on the bottom of the cell is originating from the current collector.
Also the solution in the cell retained stubbornly the faint green hypochlorite coloration during the whole run time. It is noncharacteristic and shows that there is no perchlorate being produced. In the stage where perchlorate is starting to form, the cell liquor becomes absolutely crystal clear and remains so until the end.


Like thusly:

DSCF1738.JPG - 1.1MB

Platinum plated Ti anode coupled with 316 stainless cathode in a tiny test cell on the way to ClO4- completion. The crystals on the cell bottom are sodium chlorate that formed during first stage of the run starting from chloride and dropped out due to supersaturation. By the end of the run they were dissolved and turned to perchlorate.

And a bit bigger setup I tried in a 500ml vessel also starting from sodium chloride solution and going happily way up to perch in a single run with Pt/Ti anode and SS cathode:


DSCF1745.JPG - 1021kB DSCF1751.JPG - 985kB


I managed to convert in excess of 200g of NaCl directly to perch in the 500ml cell. The solution was supersaturated and the chloride remained on the bottom until it became converted to chlorate and gradually dissolved. So direct conversion of Cl- > ClO4- can be done in a single run with Pt.


The "ubercell" although failed completely on the perchlorate stage and I can not figure out wether it was the previous conversion to ClO3- by MMO that poisoned the process....or the unfortunate lesser grade Ti on the anode stem....or the Pt deposition process.......or just plain bad luck.

Anyways I shall recoat the anode with a new Pt layer and perhaps try the direct approach again starting with PT/Ti and a chloride solution. That gig has worked repatedly, so why not this time.

markx - 3-3-2019 at 02:26

Well....the anode died officially during yesterday. With zero ClO4- having formed in the cell:



DSCF1923.JPG - 1MB DSCF1924.JPG - 1.1MB


I swapped it out to a new one which I deemed to have failed in the coating process. The surface had been poslished and could not be wetted by the hexachloroplatinic acid. It formed just some droplets, but I chucked it into the kiln anyway:



DSCF1925.JPG - 1MB


Into the cell it goes:



DSCF1926.JPG - 1MB DSCF1928.JPG - 1MB


And a miracle happens!! Lo' and behold the visual formation of the heavy perchlorate solution around the anode at the lowest voltage setting of 4,2-4,3V:



DSCF1932.JPG - 1.2MB DSCF1934.JPG - 1.2MB DSCF1931.JPG - 1.2MB

Can you see it? The haze of heavy perchlorate solution distorting the light around the anode surface and sinking down into the cell.....this is so cool!! :D

Well at least I hope it is the desired end product bending the light there. And we have definite ozone development going on, it can clearly be detected in the off gas flow.

markx - 6-3-2019 at 15:33

I discontinued the endless agony of waiting for the endproduct to form. There is clearly some kind of a pollutant in the current cell liqour batch that effectively prevents anything above ClO3- from forming.

The brief successful formation of heavy product solution that happened when I switched the anode, disappeared gradually after half hour of operation and everything went back to mere electrolysis of water as much as I could notice. There was no more ozone generation and no density changes around anode.

I tried to switch off the cell and let it cool down to room temperature to see if it was perhaps the lower temp that triggered the brief formation of perhchlorate. The cell did cool down to 20C during the previous anode change. Well, no success.
I tried to dial up and down the applied voltage to determine if there was a critical polarisation level which the anode has to reach before it can start forming pechlorate (well obviously there is :) ) but to no avail. Even applying 10V across the cell would not change things.

I just gave up on that run and removed the cell contents which have a clearly greenish blue discoloration to them. Also there is a strong presence of free chlorine and hypochlorite, which should both be pretty much gone at the stage where perchlorate formation begins. At least previous successful small scale experiments have shown it to be this way.
Most of the discoloration surely originates from the anode stem that could not resist the urge to dissolve, but I'm not completely sure it is the only culprit.
I also suspected that perhaps the anode surface texture was unsuitable. Older german literature states that only smooth Pt is suitable for electrosynthesis of perchlorate and plated or deposited Pt fails to do so, as it does not reach the critical polarisation level due to the uneven surface allowing too much charge transfer.
This may be the case, but anodes that I used in previous small scale experiments were pepared in the same way.....from the same source of Pt ....on exacly the same Ti substrate material. And they worked pretty darn good for a disposable superthin layer unit. In fact the first anode that died in this cell was deposited on the same piece of Ti I used to drive the 500ml cell to a complete "endsieg".

The only difference was that first stage conversion was performed by MMO this time and the anode stem in perhlorate stage was made from inferior Ti grade.

I'm kind of reluctant to accuse the MMO, so this leaves the contamination originating from the inferior anode stem. Mostly it should be Ti, Fe, Al, and V compounds that entered the electrolyte and perhaps found a way to fight my cause?

markx - 10-3-2019 at 05:52

I'm preparing a small test cell to find out if my previous problem was electrolyte contamination related or there is some other factor at play:



DSCF1938.JPG - 1.1MB DSCF1939.JPG - 1010kB DSCF1940.JPG - 1.1MB


Two NaClO3 solutions side by side:

DSCF1941.JPG - 1MB

The yellow one being the last problematic batch with metallic contaminants that originated from the low grade Ti shank.


Some Pb02 anodes from previous experimentation. They do shed their skin quickly in a perchlorate cell, but the Pt coat underneath shall prevail for quite some time. So I'll try one of these in the test cell:

DSCF1942.JPG - 1.1MB


Oh yeah.....for those who, like myself, think that constant current mode for a perchlorate cell sounds like a good idea:

DSCF1944.JPG - 1.2MB DSCF1943.JPG - 1.2MB

That's what's gonna happen when the power converter forces a constant current through a cell with a gradually failing anode....everything overheats, Grade 1 Ti starts to dissolve (take a look at that anode carcass on the right), cell boils dry and if one is especially lucky, bursts into flames.




[Edited on 10-3-2019 by markx]

markx - 11-3-2019 at 00:04

Quite interesting read:

Attachment: 617569.pdf (976kB)
This file has been downloaded 467 times


Seems that Pt surface needs to obtain a certain configuration for appreciable current efficacy of the process. Hence previous application history of the anode is of importance. Prepolarisation prior to perchlorate synthesis seems to have an effect on current efficacy according to the article.

I've seen similar effects when I tried the process with KClO3, due to KClO4 being mostly insoluble the formation process can be observed visually at the Pt coated anode: the perchlorate formation was always delayed, sometimes for days and then started abruptly. Sometimes on it's own and sometimes due to a rise in applied voltage across the cell.
I figured this might be due to a certain balance of compounds building up in the electrolyte, but it might just as well be that the anode surface takes it's sweet time to reach a suitable condition.
The deposited Pt is not in a condition that can be called "smooth" in an electrochemical sense. Also there is erosion taking place and it leads to an electropolishing effect, where the protruding areas shall erode away first, making the anode surface smoother. Perhaps it is required to etch away part of the Pt by the process before the surface becomes smooth enough to allow for a successful perhclorate formation to begin.

phlogiston - 11-3-2019 at 08:28

Interesting, the processes taking place at the anode are apparently a lot more complicated than I imagined.

Regarding using a constant current supply: there are also supplies that allow you to program both a current and a voltage limit. They deliver either constant-current or constant voltage, whichever is limiting.

It could be used to prevent overheating in the failure mode that you describe, because the increased resistance will lead the power supply to increase its output voltage to maintain current, untill it hits the maximum voltage setting. At that point it becomes a constant voltage supply.

markx - 12-3-2019 at 04:00

Yay!! I have definite and massive perchlorate formation going on in the small test cell. Again the formation was delayed roughly by 36 hours. During that timeframe I could not detect any perchlorate type of deposition (sudden and ultrafine) with interaction upon KCl solution. But today I get the characteristic fine deposition of cristals and there is quite a lot.

I used one of the Ti/Pt substrate lead dioxide anodes and NaClO3 solution from the clean container without the contaminants. This NaClO3 batch was also formed by the same MMO anode, so I can rule out the chlorate conversion stage of being the source of problems for further conversion.
The cell operates at about 5V and between 1-1,5A of current. The active anode surface area is roughly 8cm2, so the current density hovers around below 2kA/m2. This be on the low side for top efficacy according to literature, but I hope to stretch more life out of the poor thing this way. It has deteriorated rather healthily already.....the PbO2 skin fell off during the first hours, after which I filtered the solution to extract the lead dioxide particles. Now I can see also the Pt coating giving up in areas of greater current density. It does not so much passivate, but just dissolves away from the surface. It remains in the solution bound up by some form of a colorless complex. Letting the perchlorate solution stand for weeks after synthesis gives slow rise to a greyish slimy precipitate from the clear solution. I suspect this blob contains the platinum or at least part of it. Might try a regeneration with some aqua regia if I succeed to extract the precipitate at some point. It is really fine and tends to seep through filters.

This type of electrode deterioration is to be expected, but really I see that as a minor inconvenience. The small stock of hexachloroplatinic solution I have got is more than enough to cover a lifetime worth of Ti substrate. One literally needs a single drop to create an anode of the size I have in the small cell now.

About the CC operation mode.....yes the meltdown was caused by lack of failsafes. There sure are power supplies that have the option to preprogram all kinds of limitations, in fact I think the SEPIC converter I used "sort of" has this option available intrinsically, but I found no convenient way to check where the limitation regarding voltage up conversion kicks in at the time, so I just let er rip until the bitter end.




Side by side differences in the formation of KClO3 and KClO4 upon the action of KCl solution on cell liquors:

DSCF1945.JPG - 1.1MB DSCF1946.JPG - 1.1MB DSCF1949.JPG - 1.1MB

The right side "vial" contains a sample from the electrolyte of the small perchlorate cell and it displays the characteristic formation of KClO4 in a dense and fine layer of cristals forming instantaneously on the liquid surface where the KCl solution drop hits.
The left side "vial" contains the starting solution of NaClO3 and it displays the formation of KClO3 in a slower reaction that produces scattered coarse cristals in the solution. Just a simple qualitative method to assess if an appreciable amount of pechlorate has arisen in the cell...





[Edited on 12-3-2019 by markx]

markx - 17-3-2019 at 07:01

The small 150ml cell has been ticking along for a week now and as far as I can see it is about as good as it will get. The current flow effectively and sharply drops to a few dozen milliamps if I one lowers the cell voltage to 3,5V or below.


DSCF1967.JPG - 1.2MB


The solution has obtained the characteristic "clarity" associated with last stages of perchlorate conversion from NaClO3 and there already is visible percipitation of the product at the bottom of the cell where temperature is lower. Interestingly enough I observed basically no ozone during the whole conversion run. And the anode is still very much alive. A rather different display of events compared to what I have observed so far....successful though.






DSCF1969.JPG - 1.2MB DSCF1970.JPG - 1.2MB

On the right one can observe the amount of KClO4 that percipitated from 1ml sample of the cell liqour. The supernatant liquid (about 7ml) is water. It was added to loosen up the crystals and dissolve any chlorate or chloride that may have been present.

Sulaiman - 17-3-2019 at 08:36

Quote: Originally posted by markx  
30A worth of hydrogen shall hardly contribute to a rise in hazard level.


In one hour you would generate 30A x 3600s / (2 x[Faraday's constant]) = 0.56 moles = 12.5 litres of H2
As you wrote, not much of a hazard outside or in a well ventilated space,
but as hydrogen can detonate in hydrogen:air ratios of 1:4 to 1:59,
there is a real risk of explosion (not just fire) in a poorly ventilated environment.

e.g. worst case;
running overnight, 10 hours x 12.5 litres x 59 = total detonation in a
6' x 6' x6' room,
releasing 475 kJ/mol x 5.6 mol = 2.66x106 Joules - in milliseconds
(theoretically enough to briefly power Doc Brown's Flux Capacitor)

Just thought I'd emphasise this hazard for the benefit of less experienced chemists.
(explosions due to lead-acid battery over-charging are even now a significant risk requiring multiple mitigation implementations)

markx - 18-3-2019 at 02:13

If the cubicle one performs the synthesis in is "tighter than a duck's butt" then for sure it would not be a good idea to play around with fire in there :D

A rather more serious hazard which actually tickles the hair at the back of my neck a bit is the gas mix contained in the top part of the cell above the liquid level. If under unfavorable conditions the oxygen evolution on anode is increased, then a rather nicely detonable mix shall be contained in that volume. Even more startling is the ozone evolution stage that tends to happen at the end of perchlorate conversion stages. The current collectors run through that volume of gas. If they are undersized for the amount of current that they have to commute or there is a bad connection in there.....overheating.....bang.
I have not actually heard of such a thing happening regarding electrosynthesis of the compounds covered here, but the possibility is there. And I know from first hand experience that even moderate amounts of hydrogen mixtures with that composition can do a lot of bad things if confined in a reactor.

markx - 25-3-2019 at 11:01

I'm performing a second run with the small cell and a set of anodes I made at different Pt deposition temperatures (pyrolysis temperatures more precisely).

The cell has been running for 6 days now and there are massive sodium chlorate crystals on the bottom. They tend to drop out in an intermediate stage of the conversion where both perchlorate and chlorate are present in a healthy concentration. At the end of the conversion they dissolve again.

DSCF1984.JPG - 1.2MB DSCF1988.JPG - 1.2MB


The set of small anodes I made to investigate the effect of Pt deposition temperature on the longevity of the anode:


DSCF1990.JPG - 1.2MB DSCF1989.JPG - 1.2MB

I varied the temperature from 250C - 400C and also varied the number of coats applied : either 1 or 4 coats of Pt.

The procedure that constituted one coating of Pt applied, was as follows:

Grade 1 Ti strips that were previously sanded clean with 400 grit wet dry paper and stored under ethyl alcohol were dried and coated with hexachloroplatinic acid solution. They were just wiped with a drop of the solution and as much as remained on the surface in a uniform manner was left there. Excess was removed. The electrode was then placed on a fixture and into a preheated temperature controlled laboratoory kiln for 10 minutes. After the 10 minutes were up, the electrode was removed from kiln and cooled down. It was flushed with water and wiped with ethyl alcohol to remove any loose Pt particles. After that a "coating" was deemed to have been applied. The procedure was repeated at the same temperature to apply multiple coats.

The set I prepared was as follows:
250C 1 coat
250C 4 coats
300C 1 coat
300C 4 coats
350C 4 coats
400C 1 coat

The cell was loaded with 150ml of NaClO3 solution and electrolysis was commenced at 4,3-4,6V and a current of 0,7-0,8A. The anodes have a surface area of about 8cm2. So the current density is in the range of 100mA/cm2. Abit on the low side, but otherwise the cell temperature creeps up too far.
I started off the conversion run with 250C 1 coat anode: it was not durable and perished wihin the first 3 hours of operation due to passivation.
After that the 400C 1 coat anode was put to use and it showed markedly better resistance against passivation. It persisted for four days in the cell, before noticeable passivation occurred. For practical purposes I could have stretched one more day out that one, but I opted to change it to 350C 4 coats specimen.

That one has been bubbling away for 2 days now and for all intentive purposes does not yet show noticeable passivation.

Seems that it makes sense to try even higher Pt deposition temperatures....say in the range of up to 800C. I was afraid that higher temperatures would increase the formation of oxide coating underneath the Pt layer and render the anode less effective, but current results show a reversed trend. At least up to a certain point I guess.





MrHomeScientist - 25-3-2019 at 13:11

This is fantastic work; really great to read. Your cell construction looks very nice, and makes me yearn even more for a shop with those sorts of tools. Out of curiosity, what is the end use for all this perchlorate?

Loptr - 25-3-2019 at 13:28

Wow, I can't believe I missed this thread. Very nice construction!

markx - 25-3-2019 at 14:36

Quote: Originally posted by MrHomeScientist  
This is fantastic work; really great to read. Your cell construction looks very nice, and makes me yearn even more for a shop with those sorts of tools. Out of curiosity, what is the end use for all this perchlorate?


Thanks for the kind words! :) Really, there is no "end use" of any particular purpose for this project. Just doing it to expand the extent of my knowledge sphere. Perhaps I'll try some visco compositions based on perchlorate to yield a clean burning fuse without much soot and dross. As a matter of fact the accumulation of product from the "ubercell" would be a real problem.

MrHomeScientist - 4-4-2019 at 11:37

I can definitely get on board with that! Nothing wrong with doing things for fun and learning.
I find it interesting that there are a ton of people out there making chlorate and perchlorate cells to create mountains of these chemicals, but I rarely see what anyone's making them for. Pyrotechnics, I guess?

markx - 11-4-2019 at 09:39

Been tinkering with the small cell and higher deposition temperatures involved in the anode making while I wait for my grade 1 Ti rod to arrive, so I can revive the ubercell.

I went ut to 600C for the Pt deposition temperature and prepared a set to test out how the coats perform.



IMG_3314.JPG - 794kB

IMG_3315.JPG - 686kB IMG_3316.JPG - 630kB IMG_3317.JPG - 669kB

Cleaning of spent anode substrates and storage under alcohol prior to recoat




IMG_3319.JPG - 657kB IMG_3324.JPG - 878kB IMG_3326.JPG - 1MB

Heating up the kiln with the stand to hang the anodes from in it.



IMG_3329.JPG - 555kB IMG_3334.JPG - 910kB IMG_3335.JPG - 649kB

Applying a thin layer of hexachloroplatinic solution on substrate. Into the kiln for 10min and out they come again...




IMG_3340.JPG - 850kB

Final set of 500C 1 coat, 500C 4 coat and the same for 600C.


I did start the testing with the 600C 1 coat anode to see how it comapres to the 400C counterpart that endured for four days before giving up the ghost.
All conditions being reasonably repeateable the 600C specimen endured for 6 days and some exta hours before passivation set in. Not bad....the 400C counterpart stretched 4 days of life out of it. So a day for every 100C raise in deposition temperature :D


DSCF2001.JPG - 1.2MB DSCF2004.JPG - 1.2MB DSCF2006.JPG - 1.2MB DSCF2007.JPG - 1.2MB

Passivation...only a few spots are seen to bubble on the anode. But the PT coating seems to be mostly there, just it has a TiO2 coat underneath that prevents it from conducting.




DSCF2008.JPG - 1.2MB DSCF2009.JPG - 1.2MB DSCF2011.JPG - 1.2MB

600C 4 coats anode goes in and the surface conducts evenly. In fact I had to dial down the voltage to 4,5V as the cell heated up and current creeped above 1,2A at 4,8V. This is too much for the little plastic pot and it shall boil up. Now the 600C 4coat has been ticking along for 3 days at 0,8-0,9A and everything is stable.

The 350C 4 coat anode that I used to finalize the previous conversion run was working without any signs of passivation for 8 days until the chlorate became compeltely depleted and then it abruptly and totally passivated. It happened within one hour of operation and the deterioration was devastatingly complete. It further cements my conclusion that most of the damage to the anode shall happen at the last stages of conversion.

But for the life of me I have not noticed even a hint of real ozone production from the current small cell....that is strange. Because I remember the small cell that I ran with similar anodes (made with not precicely controlled deposition temperature) previously, produced so much ozone that it one could smell it two rooms away.

hissingnoise - 11-4-2019 at 11:23

Your amber liquid looks like my filtered cell-solution after a 30 hour run and a half-eaten cheap oiled graphite rod...


markx - 11-4-2019 at 13:10

Quote: Originally posted by hissingnoise  
Your amber liquid looks like my filtered cell-solution after a 30 hour run and a half-eaten cheap oiled graphite rod...



Totally different animal though! :D

Come to think of it.....years ago when I saved this dangerous amber beauty from disposal I thought that I shall likely never find a reasonable use for it. In fact I mostly took it for the fancy bottle.....how wrong I was.

Photonic - 14-4-2019 at 12:05

For those investigating plating of platinum to titanium, or plating anything to titanium in general it is a fickle beast. One of the best references I have found as of yet is the ASM Handbook Volume 5 - Surface Engineering.

It has some good information on plating solutions, recommended rinse methods, prep, etc.

markx - 18-4-2019 at 07:59

Some update on progress.....I tried to kill the 600C 4 coat anode by letting it run the cell to full conversion and beyond as far as could be perceived. The poor thing was ticking along in the cell at 4,5-4,6V and 0,7-0,8A for three days, then chlorate depletion set in and current dropped to 0,3A. I let the torture continue for 7 more days in hopes of reaching the end for this Pt deposit. Aaaaaand, it does not die, nor wear, nor passivate! :D
I gave up on that one, dumped the cell contents to collecting flask and charged a fresh chlorate solution into the cell. At 4,4V I get 0,85-0,9A current flowing, depending on how good the alligator clips manage to connect to the electrodes and the whole surface is working like brand new. This is amazing....it means that the anode survived a full conversion and depleted cell conditions without a hint of passivation. That is a first, usually I go through two anodes in a conversion run. The first one tends to die close to 3/4 th conversion and the second one ususally at the very end if chlorate becomes depleted. But the 600C 4 coat survived without a damage and is currently processing a second conversion. I think this might be very close to a sweet spot regarding the Pt deposition parameters. Let's see how far we can stretch this specimen :)

markx - 24-4-2019 at 13:04


Methylene blue has arrived.....surely a lifetime supply for pennies:

57798830_394400864480478_3304869350204243968_n.jpg - 69kB



Strong presence of perchlorate is indicated in the second conversion run of the 600C 4 coat anode

57798784_2211132398941398_5026436248399511552_n.jpg - 62kB

In fact the second conversion run is nearing a rather end stage and the anode shows no signs of degradation. It is running strong at 4,7V and 1A. Defiantely this specimen is the most succesful anode attempt that I've managed to conjure so far.

markx - 5-5-2019 at 23:22

The 600C 4 coat anode died at last......after accomplishing three full conversions of a total volume of 500ml concentrated sodium chlorate stock solution. Likely even a bit more than 500ml as I added stock to the cell to replenish the losses during runs and it amounts definately more to 50ml excess in total. Did not register the total amount of the additional chlorate stock, but then again I was just trying to find out how long the electrode would last. The anode has been working constantly from the 5th of April until today, 6th of May. Minus the time it was off during recharging the cell inbetween conversion batches, but that sums to a total of few hours at best.

A grand total of roughly 700h of operation in rather loosely controlled perchlorate cell conditions before It gave up the ghost. I think it is a remarkable result for something with such a fragile and thin Pt coating. I must note that the first signs of degradation could be noticed at about midway through the last conversion, so the specimen has been outstandingly rugged compared to previous ones that were deposited at a lower kiln temperature.

I think it is time to execute the same deposition conditions on a larger substrate and try this with a scaled up version in the bigger cell. Shame the Ti rod for the current collector has not yet arrived and I can not fabricate an operational setup, but the active surfaces can be prepared in advance :)

I shall percipitate the converted solution stock with KCl and measure the total yield. Or try with a smaller sample from the combined stock and extrapolate for the total volume/mass. I really have no immediate need for KClO4, so might as well keep it in the solution form for any further ideas I might come up with.

markx - 8-5-2019 at 03:27

The Ti rods arrived, so I proceeded to fabricate a new anode stem for the "ubercell":

IMG_3518.JPG - 75kB IMG_3520.JPG - 80kB IMG_3521.JPG - 80kB IMG_3523.JPG - 96kB IMG_3524.JPG - 74kB IMG_3527.JPG - 82kB IMG_3529.JPG - 80kB IMG_3531.JPG - 78kB IMG_3533.JPG - 118kB

It should be at least grade 2 Ti by the looks and feels of it. Machines easily, is soft and pretty much ok to tap. I suspect the previous rod that I used as anode stem was from grade 5 (alloyed Ti) and that material was tough as a coffin nail. Near to impossible for any tapping operations. By extreme carefulness and a lot of prayer I succeeded, but it's not an experience that I would love to repeat. Well, let's see if it holds up in the cell under anodic potential....

As for the active part of the anode I took a spent substrate from last time and cleaned it by sanding. Then deposited 5 coatings of Pt to it at 600C in the lab kiln. Inbetween every coating the anode was wiped clean with a moist paper and then with alcohol until no more loose Pt could be detected on the paper towel. The first coating had the most content of loose Pt dust, but from the third one forward there was literally nothing that could be wiped off:



IMG_3537.JPG - 82kB IMG_3538.JPG - 89kB IMG_3539.JPG - 112kB IMG_3541.JPG - 83kB IMG_3542.JPG - 86kB IMG_3544.JPG - 68kB IMG_3546.JPG - 80kB IMG_3548.JPG - 67kB IMG_3549.JPG - 93kB IMG_3550.JPG - 77kB IMG_3551.JPG - 82kB IMG_3552.JPG - 80kB

The Ti plate was attached to the slit end of the stem by compression fitting. It is pretty "goodentoit", but removable upon request and against my intrinsic suspicions this type of connection seemed to work without passivation in the cell. At least it did so with the previous anode stem.


Charged into "ubercell" (the main conversion run with 600C 5 coat anode begins 08.05.19):

IMG_3555.JPG - 110kB IMG_3553.JPG - 118kB IMG_3557.JPG - 118kB IMG_3558.JPG - 116kB

[Edited on 8-5-2019 by markx]

markx - 13-5-2019 at 09:53

Zooo....the contrapulation has been fizzing away on my tabletop for about 5 days now. The anode stem is not corroding, the anode has not passivated and conducts very nicely and we have indication of perchlorate in the cell liqour. Both tests, methylene blue solution and percipitation by KCl show the presence of perchlorate:

DSCF2031.JPG - 1.1MB


I did upgrade to larger cathodes as the stumps I had in there did hinder the process to such degree that I could only get 4,5A through the cell at best. This will not do in terms of time expenditure....it would take forever to convert that load in the cell. So in went the large Ti cathode plates I use for chlorate runs. I also made special Ti "bolts" to secure the plates to stems and a key to fasten them:


IMG_3565.JPG - 725kB IMG_3567.JPG - 778kB IMG_3569.JPG - 696kB IMG_3573.JPG - 682kB IMG_3579.JPG - 947kB IMG_3580.JPG - 850kB IMG_3583.JPG - 882kB


That's more like it....10 amps and temperature around 50C. I try to keep it around this mark as it is a safe middle ground. No excessive heating, but still reasonable productivity. The liqour is quite clean as can be seen, so nothing of contaminative character seems to have dissolved into the electrolyte. Seems to work out this time...

DSCF2038.JPG - 1.1MB DSCF2039.JPG - 1.2MB DSCF2035.JPG - 1.2MB

markx - 15-5-2019 at 15:15

It is coming along very nicely. ClO4- content is growing steadily as recognized from precipitation test results. Ozone can be detected in off gas flow, not much but it is clearly noticeable.


The titianium bolts securing cathode plates to the stems:

DSCF2045.JPG - 1.2MB

Anode edges can be seen to have lost conductivity (the darker rim around anode bottom part):

DSCF2048.JPG - 1.2MB

Not too bad though, the overall conductivity is very good:


DSCF2051.JPG - 1.1MB DSCF2052.JPG - 1.2MB

The electrolyte is very clear and translucent. It has lost the greenish hypochlorite tinge, a telltale sign that the convesion is going well and has reached a stage where perchlorate content has become prevalent.

There is offensive salt creep down the sides of the cell, clearly the seal at the top of the cell needs improvement, but this is more of a cosmetic issue.

[Edited on 15-5-2019 by markx]

markx - 16-5-2019 at 04:18

I did measure the KClO4 yield in the collected liqour from the small 150ml cell conversion runs and it came close to 0,9g/ml.....pretty thick stuff :D

2 glass vials were cleaned, dried and weighed to establish tare mass. Then 2ml of collected cell liqour was inserted into one vial and weighed to 0,01g accuracy.

Density of the cell liqour was established as 1,5ml/cm3

6ml of saturated KCl soln. was added to the 2ml cell liqour sample to precipitate the product. 8ml of distilled water was added into the vial to loosen up the cristalline layer and to enable it to separate from the liquid phase.

The liquid phase was removed with a syringe and needle to the maximum possible extent. Some of the precipitate was sucked along with the liquid. This was injected into second vial an let settle. From second vial the liquid phase was again removed after the layer settled and then discarded. The main precipitate was once again washed with 2ml of distilled water that was again removed with the syringe.
The vials were carefully microwaved to dry the precipitate and then weighed again.
The collective mass of preciptate from both vials summed as 1,8g.

I also measured the collective volume of cell liqour from the 150ml runs and it sums up to 610ml total weighing in at 913g d=1,49g/ml

The total expected yield when converted to KClO4 from this amount of liquor would be around 550g. Depending on how much losses occur at purification.
That is the result of a month worth of electrolysis with the small cell running at an average guestimate of 0,6A.

If my very ragged calculations hold any water then this would amount to about 50,smt% current efficacy?

[Edited on 16-5-2019 by markx]

[Edited on 16-5-2019 by markx]

markx - 25-5-2019 at 01:25

She's clearly cooked and done (08.05.19-24.05.19):



DSCF2056.JPG - 1.2MB DSCF2057.JPG - 1.1MB DSCF2058.JPG - 1.2MB DSCF2059.JPG - 1.2MB

DSCF2060.JPG - 1.1MB DSCF2061.JPG - 1.2MB DSCF2065.JPG - 1.1MB


The cell liquid had obtained a deep clarity with almost a vitreous bluish tinge. High refractive index can be observed, characteristic of a concentrated solution. Further torture is meaningless and shall only manifest itselt in electrolytic discharge of water and bringing the anode closer to death.

I carefully suctioned the contents of the cell into a holding canister and discarded about 50ml that contained the slimy haze at the cell bottom.

The contents of the cell weigh in at 3672g by a volume of 2,5l. I visually assess that about 75-80% of anode surface is still active, so it should be good for one further conversion of same magnitude.

Lets find out:




DSCF2067.JPG - 1.1MB DSCF2068.JPG - 1.2MB DSCF2069.JPG - 1.2MB

markx - 3-6-2019 at 00:13

The second conversion is done.....so is the anode. I let it cook until it passivated completely at the maximum of 5,4V from the power supply. Also the thermometer coupling disintegrated where the threading used to be for mounting it to the cell cover. The plastic electrode couplings also seem to turn into slime. Nothing short of PTFE or PE is going to hold up very long in them fumes. But it finished 2 "ubercell" conversions with one anode, totaling guesstimatively above 4kg of KClO4 and that is not too shabby at all!
It is time for an overhaul regarding the couplings and this time I aim for full PTFE set. Also a more effective seal for the cell cover is needed. The makeshift plumber tape wound contraption is not really tight and has considerable salt creep+ some of the gas leaks out. Luckily it does seal against the mist, but evident improvement is needed.

The second conversion was done with the contaminated sodium chlorate batch from first attempt that did not want to form any perchlorate with the old (grade 5?) Ti anode stem. In fact it had formed some perchlorate after all as it turned out. It was faintly indicated with the methylene blue test, but not enough to be indicated by the precipitation test with KCl. By the time I was running that batch, I had no methylene blue, so I could not detect the faint presence of product. I filtered the goop out from the stored solution and gave it a try with the new anode setup. Worked beautifully the second time and it was quicker than the first conversion.
So it seems my suspicions about the metallic contaminants from the dissolved anode stem hindering the conversion were unfounded. I guess the problem was more likely of electrochemical nature (dissolution of the anode stem pulling down the anode potential enough to keep perchlorate formation at a minimum?)....or the chlorate conversion was incomplete to begin with and it just took way longer than I had the patience to endure.

So far, so horrible.....but what the hell am I going to use the product for now?


I replaced the tired plastic couplings with a set I machined from PTFE stock.......should be way more durable:
DSCF2071.JPG - 1.2MB DSCF2072.JPG - 1.2MB DSCF2073.JPG - 1.2MB DSCF2070.JPG - 1.2MB



The second conversion batch weighs in at 4111g at about 2,75l capacity:

DSCF2074.JPG - 1.2MB DSCF2075.JPG - 1MB


A sample of 205g of the NaClO4 liqour was taken ans subjected to percipitation with saturated KCl solution:

DSCF2079.JPG - 1.2MB DSCF2080.JPG - 1.2MB DSCF2084.JPG - 1.2MB


The product was filtered on a glass frit :



DSCF2086.JPG - 1.2MB

[Edited on 3-6-2019 by markx]

[Edited on 3-6-2019 by markx]

markx - 5-6-2019 at 08:30

The yield from the 205g (135ml) stock solution when converted into KClO4:



DSCF2089.JPG - 1.1MB DSCF2090.JPG - 1.2MB

markx - 6-6-2019 at 12:27

I did spin some visco based on the KClO4:



DSCF2091.JPG - 1.1MB DSCF2092.JPG - 1.2MB DSCF2093.JPG - 1.2MB


I am utterly unimpressed so far.....for something that required so much effort and fun to produce on my tabletop from scratch, it really performs no wonders on it's own. But I guess that has more to do with the preparation (or the lack of) of the fuse composition.

I took a very simple approach: 75/25 KClO4/C (charcoal)
Ingredients were milled in electrical coffee grinder (obviously in separated turns) and mixed together in a bowl. 5-7% EtOH was added to the mix and it was screened twice through a fine sieve (0,5mm) to yield a slightly granulated powder. It was allowed to dry completely in the sun for 2 hours and then spun into fuse. The fuse was coated twice with diluted contact glue. A standard method I use also to coat BP based fuse. It yields a durable flexible and waterproof product.

Well it does burn.....rather consistently, but :
really hard to light
not very agressive
still a lot of dross (not nearly overoxydised enough to burn away the threads)

I mean sure it was a halfbaked approach, but I expected at least some kind of wow effect :D
At least it does not stink of sulfur....

markx - 10-6-2019 at 01:20

I also tried 87/13 and 65/35 ratios KClO4/C respectively. These do not burn at all or do so very slowly and tend to go out by their own.
So the workable range for visco I guess is at about 75-80/25-20.....

Still I am amazed at how feebly the perchlorate performs as an oxydizer....at least in a mix with just carbon. Chlorate in the same mixture is exceedingly energetic and violent, even when the mixture is coarse and not well homogenized. But the sensitivity ruins the noble cause.

Perhaps if the the ingredients were ball milled to incorporate them into each other more thoroughly as can be done with BP based formulations. But I'm not eager to try it with perchlorate, to be honest. Although it seems to be quite impossible to ignite the perch/C mix with a hammer blow, but still a very imminent danger of a mishap is there.

yobbo II - 10-6-2019 at 05:01

Perchlorate is much more stable than chlorate

markx - 10-6-2019 at 07:22

Quote: Originally posted by yobbo II  
Perchlorate is much more stable than chlorate


Indeed it is....but I clearly did not expect the difference to be that drastic.

markx - 17-6-2019 at 04:49

Jeez....the simple K perchlorate+reducer mixtures seem so feeble and anemic because of the high decomposition temperature of the potassium salt that I really see no possibility to use them straight as a core filling for visco. Also the usual accelerators for decomposition seem not to work on KClO4.

Interestingly a chinese patent ( CN101337855A ) describes a more complex mixture that overcomes the problem of high activation energy and slow decomposition kinetics of KClO4.
Namely with the addition of 2-8 parts of K nitrate, 5-8 parts of Ca sulfate and up to 8 parts Ca carbonate as accelerants. Seems worth a try as I tend to have all of these components at hand.

markx - 20-7-2019 at 02:24

I finally managed to devise a way to make the perchlorate work effectively in fuse formulations: the key is in preparation of the mix. It absolutely needs a very intimate contact with the fuel, just like black powder based formulations.
There are two major ways to accomplish this in an amateur setting:
a) (ball) milling the mix- not viable for perchlorate formulations (at least my selfpreservation instinct does not allow it)
b) impregnating fuel by a perchlorate rich solution to form crystals in and around the fuel particles

I chose the second option. I made a small 2g sample of 75/25 KClO4/C, but this time I changed the preparation process to try out a "vaccum assisted preparation" idea:



Ingredients were weighed into a small glass dish and 0,5ml of azeotropic EtOH +1ml water was added. The alcohol serves the purpose of lowering surface tension to yield better wetting effect of carbon.

The ingredients were mixed with a spoon until uniform (a few minutes) and compacted into a solid cake. The consistency of the mix was like damp dirt so it stuck together nicely.

After that the sample was placed into a vaccum chamber and evacuated for 30 minutes at room temperature (20C). Then the sample was taken out, the cake broken up into loose rubble and put back into the chamber. Another session of 30 minutes under reduced pressure and slight warming at 40C yielded a semi dry granulated product. It was still damp, but good enough to test for burning speed.

A small lump of the prepared mix was collected onto a stainless spoon and ignited with a butane torch: the sample burned with satisfactory violence and was energetic enough to flying the burning lump off the spoon. Definitely the uniformity and vigor of the burn has been improved by the vaccum assisted preparation process.

The slightly damp mix was granulated by forcing through a fine sieve and let completely dry at room temperature and atmospheric pressure (24h).

The sample was spun into a lenght of fuse after it had been dried:



DSCF2094.JPG - 954kB DSCF2095.JPG - 1MB



It works just beautifully now! A nice hot, energetic burn that proceeds at an even pace with a sharp long flame jet and a powerful hiss. I'm very satisfied with the outcome.



2019_07_20T10_33_26_452Z.jpeg - 1.7MB 2019_07_20T10_33_59_247Z.jpeg - 1.9MB 2019_07_20T10_34_10_025Z.jpeg - 2.4MB

[Edited on 20-7-2019 by markx]

Raniphad - 25-7-2019 at 23:30

Great Information.

underground - 6-8-2019 at 16:14

Markx i got an MMO electrode and i want to spot weld to it a titanium bar for delivering the current. I have not any spot welder tho and i was thinking to use some electrolytic caps in parallel, charge them, and spot weld it. What do you think, is it going to work ? I have seen some videos that some doing it with a super-capacitor.

[Edited on 7-8-2019 by underground]

markx - 6-8-2019 at 22:43

Quote: Originally posted by underground  
Markx i got an MMO electrode and i want to spot weld to it a titanium bar for delivering the current. I have not any spot welder tho and i was thinking to use some electrolytic caps in parallel, charge them, and spot weld it. What do you think, is it going to work ? I have seen some videos that some doing it with a super-capacitor.

[Edited on 7-8-2019 by underground]


Given enough capacity it will likely work, but I would think it takes a "bit" of tinkering around to get the parameters just right.
You could also try the compression fitting method I used with my perchlorate anode. Just squeeze the MMO mesh into a slot on the anode stem....additionally one could compress it further with a Ti bolt e.g. It worked just fine without a bolt for me, despite my initial fear that the connection spot would passivate in minutes rendering the system incapacitated. If such a connection will hold up in perchlorate cell conditions, then I would believe it works well also in chlorate setups.